Laporkan Masalah

PENGARUH TEKNIK PENCETAKAN DENGAN BAHAN POLYVINYL SILOXANE DAN WAKTU PENGISIAN TERHADAP STABILITAS DIMENSI FINISHING LINE DAN ANTAR FINISHING LINE MODEL GIGI TIRUAN CEKAT

PAMBUDI SANTOSO TANZIL, drg. Endang Wahyuningtyas, M.S., Sp.Pros (K)

2014 | Tesis | S2 Prostodonsia

Stabilitas dimensi finishing line merupakan hal yang penting dalam menentukan keberhasilan perawatan gigi tiruan cekat. Polyvinyl siloxane merupakan salah satu bahan cetak yang memiliki stabilitas dimensi yang sangat baik. Teknik pencetakan dengan bahan polyvinyl siloxane dan waktu pengisian merupakan faktor yang mempengaruhi stabilitas dimensi finishing line dan antar finishing line gigi tiruan cekat.Tujuan penelitian ini adalah untuk mengetahui pengaruh teknik pencetakan dengan bahan polyvinyl siloxane dan waktu pengisian terhadap stabilitas dimensi finishing line dan antar finishing line model gigi tiruan cekat. Penelitian ini dilakukan pada 36 sampel model kerja gigi tiruan cekat, dibuat dari hasil cetakan dengan bahan polyvinyl siloxane yang diisi dengan gips tipe IV. Sampel dibagi menjadi 6 kelompok, yang terdiri dari 6 sampel dalam tiap kelompok. 3 kelompok dicetak dengan teknik one step, dan 3 kelompok berikutnya dengan teknik two step. Masing-masing kelompok teknik pencetakan diisi setelah 2 jam, 30 jam, dan 58 jam. Setelah sampel selesai dibuat sesuai dengan ketentuannya, seluruh sampel discan dengan 3D laser scanner (Ceramil Map-400, Amanngirrbach, Germany). Kemudian diukur jarak finishing line dan antar finishing line dengan menggunakan software 3D Tool. Data dianalisis dengan Anova dua jalur dan dilanjutkan uji Post-Hoc Least Significant Difference (LSD). Hasil penelitian menunjukkan bahwa: 1) Terdapat perbedaan yang bermakna antara kelompok 30 jam one step, 58 jam one step, dan 58 jam two step dengan master model pada lebar finishing line (p<0,05); 2). Terdapat perbedaan yang bermakna antara kelompok 30 jam one step, 30 jam two step, 58 jam one step, dan 58 jam two step dengan master model pada lebar antar finishing line (p<0,05). Kesimpulan dari penelitian ini adalah: 1) Teknik pencetakan dengan bahan polyvinyl siloxane berpengaruh terhadap stabilitas dimensi finishing line dan antar finishing line model GTC. Teknik pencetakan two step dengan bahan polyvinyl siloxane menunjukkan stabilitas dimensi yang lebih baik daripada teknik pencetakan one step setelah 2 jam pengisian pada finishing line dan antar finishing line model GTC; 2) Waktu pengisian cetakan polyvinyl siloxane menurunkan stabilitas dimensi finishing line dan antar finishing line model GTC. Waktu pengisian cetakan polyvinyl siloxane 2 jam menunjukkan stabilitas dimensi yang terbaik pada finishing line dan antar finishing line model GTC.

Dimensional stability is the important key in determining the success of fixed partial denture treatment. Polyvinyl siloxane is one of the impression material with best dimensional stability. The impression technique and the pouring time of polyvinyl siloxane material are the factors that will influence the dimensional stability of fixed partial denture finishing line and the distance between finishing line. The aim of this study was to investigate the effect of pouring time and impression with polyvinyl siloxane as material related with dimensional stability fixed partial denture finishing line and the distance between finishing line. This research run on 36 working model samples of fixed partial denture which were made from polyvinyl siloxane filled with type IV gypsum. The sample divided into 6 groups consist of 6 samples for each group. The groups also classified as 3 groups with one step impression technique and the other three with two steps impression technique. Each of the impression technique group poured after certain time; after 2 hours, 30 hours, and 58 hours. After the sample precisely made by following the procedures, it scanned with 3D laser scanner (Ceramil Map-400, Amanngirrbach, Germany), then the distance between finishing lines measured with 3D tool software. Finally, all collected data analyzed with two way Anova and proceed with Least Significant Difference (LSD) test. The results showed that: 1) There was a significant difference between the one step 30 hours, one step 58 hours, and two step 58 hours groups with the master model at the finishing line width (p <0.05); 2) There was a significant difference between the one step 30 hours, two step 30 hours, one step 58 hours, and two step 58 hours groups with the master model at the distance between finishing line (p <0.05). The conclusions of this study were: 1) Impression technique with polyvinyl siloxane material had effect on dimensional stability of fixed partial denture model finishing line. 2 hours impression pouring time with two steps impression technique and polyvinil siloxane as material shows better dimensional stability than one step impression technique with same pouring time and same material in fixed partial denture model finishing line.2) Pouring time polyvinyl siloxane decrease the dimensional stability of fixed partial denture model finishing line. The 2 hours impression pouring time polyvinyl siloxane shows the best dimensional stability of fixed partial denture model finishing line and the distance between finishing line.

Kata Kunci : Stabilitas dimensi finishing line merupakan hal yang penting dalam menentukan keberhasilan perawatan gigi tiruan cekat. Polyvinyl siloxane merupakan salah satu bahan cetak yang memiliki stabilitas dimensi yang sangat baik. Teknik pen


    Tidak tersedia file untuk ditampilkan ke publik.