Optimalisasi parameter proses dalam stereolithografi pada pembuatan stainless steel berporus

SUKMAJI INDRO CAHYONO, Ir. Muslim Mahardika, ST, M.Eng., Ph.D.,IPM,. ASEAN.Eng ; Dr. Ir. Budi Arifvianto, S.T., M.Biotech ; Prof. Dr. Suyitno, ST, M.Sc

2026 | Disertasi | S3 Teknik Mesin

Stereolitografi generasi kedua, Digital Light Processing (DLP) menawarkan pendekatan yang menjanjikan untuk fabrikasi komponen logam dengan geometri kompleks. Namun, produksi komponen dari baja tahan karat yang berpori, masih menghadapi tantangan akibat keterkaitan antara formulasi slurry, akurasi pencetakan, debinding, dan sintering. Penelitian ini mengkaji optimasi parameter proses dalam pembuatan struktur baja tahan karat 316L berpori menggunakan printer DLP komersial. Studi ini mencakup tiga tahap utama: pra-pemrosesan (distribusi ukuran serbuk dan fraksi berat campuran), proses pencetakan (ketebalan lapisan, waktu paparan, dan kekasaran film FEP), serta pasca-pemrosesan (debinding, sintering, dan sensitisasi).

Hasil eksperimen menunjukkan bahwa serbuk 316L berbentuk bola bulat hasil atomisasi gas dengan ukuran partikel rata-rata 28,25 m mampu menghasilkan pembentukan lapisan yang relatif stabil. Variasi kandungan serbuk (25–75 wt%) meningkatkan densitas dan ikatan antarpartikel, namun menurunkan transmitansi cahaya sehingga membatasi efisiensi curing dan berpotensi melemahkan ikatan antar lapisan. Tantangan utama pasca-pemrosesan meliputi stabilitas geometri selama debinding dan sintering, di mana penghilangan binder dan penyusutan termal memengaruhi mikrostruktur akhir serta kemurnian material.

Selain itu, metode Resin Exposure Range Finder (RERF) dan desain ortogonal Taguchi L9 digunakan untuk mengidentifikasi parameter pencetakan paling berpengaruh. Pada geometri tonjolan (protrusion), ketebalan lapisan menjadi faktor dominan dengan kondisi optimal 0,05 mm, waktu paparan 6 s, dan kekasaran FEP 1,4 m. Sedangkan pada geometri cekungan (indentation), waktu paparan paling berpengaruh dengan kondisi optimal 2,5 s, kekasaran FEP 0,59 m, dan ketebalan lapisan 0,2 mm. selain itu, overpolimerisasi akibat hamburan cahaya menyebabkan pertumbuhan geometri berlebih, terutama pada jarak celah 30–70 m dan dosis energi di atas 500 mJ/cm².

Digital light processing (DLP)-based stereolithography offers a promising route for fabricating  metallic components with complex geometries; however, the production of dense, porous stainless  steel parts remains challenging due to interrelated issues in slurry formulation, printing accuracy,  debinding, and sintering. The research investigates the optimization of process parameters for  manufacturing porous 316L stainless steel structures using a commercial DLP printer. The study  addresses three main stages: pre-processing (powder size distribution, and solid loading), printing (layer thickness, exposure time, and FEP film roughness), and post-processing (debinding, sintering, and sensitization).


Experimental results demonstrate that spherical gas-atomized 316L powder with a mean particle  size of 28.25 m enables stable layer formation. Furthermore, the influence of stainless steel  powder content (25–75 wt%) on printability and sinterability was examined. Increasing powder  concentration enhances density and interparticle bonding but reduces light transmittance, thereby  limiting curing efficiency and potentially compromising interlayer adhesion. The study also  addresses key challenges in post-processing, particularly maintaining geometric stability during  debinding and sintering, where binder removal and thermal shrinkage critically affect the final microstructure and purity of the metallic product.

Additionally, using the Resin Exposure Range Finder (RERF) method and Taguchi L9 orthogonal  array, the most influential printing parameters were identified. For protrusion geometries, layer  thickness is the dominant factor, with optimal conditions of 0.05 mm layer thickness, 6 s exposure  time, and FEP roughness of 1.4 m. For indentation geometries, exposure time exerts the greatest  influence, with optimal settings of 2.5 s exposure time, 0.59 m FEP roughness, and 0.2mm layer  thickness. Over-polymerization due to light scattering leads to geometric overgrowth, which  becomes critical at gap distances of 30–70 ?m and energy doses above 500 mJ/cm².

 Finally, the post-sintering analysis reveals that residual carbon from the PLA-based photopolymer  promotes sensitization, evidenced by the formation of chromium carbides (Cr-C) and carbon  contents of 6–8 wt?r exceeding the 0.03 wt% typical of 316L stainless steel. This sensitization  depletes chromium at grain boundaries, compromising corrosion resistance. SEM-EDX mapping  confirms the co-localization of chromium and carbon, and dangling fiber-like structures on sintered surfaces corrosion due to the chromium depletion into chromium carbide compond. 

Kata Kunci : Digital light processing, porous stainless steel, sensitization, Taguchi method, additive manufacturing.